Home > Blog > Content

How are titanium rods produced? Part 8:Titanium Rod Inspection

Dec 31, 2025

The inspection of titanium rods after grinding is divided into two categories: industrial-grade titanium rods and medical-grade titanium rods. The requirements for medical-grade rods are several times more stringent than those for industrial-grade rods. The core process follows the sequence of "appearance inspection → dimensional inspection → physical/chemical/non-destructive testing → final inspection and release." Each step has clear acceptance criteria and testing methods. The following are the detailed steps (including key parameters, testing tools, and acceptance thresholds, adapted for production implementation).

Complete inspection process for medical-grade titanium rods after grinding (rigorous level, 100% full inspection)

Medical-grade titanium rods, after grinding, must meet the requirements of "sterility, defect-free, and biocompatibility." This involves several additional specialized tests beyond those for industrial-grade titanium, and the process consists of eight steps, all of which are essential.

Step 1: Visual Inspection (Initial inspection, quickly screening out obvious defects)
Inspection Tools: Visual inspection (naked eye + 5x magnifying glass)
Inspection Content and Acceptance Criteria:
Surface Defects: No cracks, folds, scratches, sand adhesion, oxidation discoloration, grinding burns (burns appear as blue/yellow/black spots, strictly prohibited), no residual grinding debris or burrs.
Judgment: Any visually visible defect is considered non-conforming and should be marked for rework (re-grinding or touch-up grinding).

Step 2: Surface Roughness Inspection (Core Accuracy Indicator)
Inspection Tool: Portable surface roughness tester (accuracy ≥ 0.001μm)
Inspection Rules:
Inspection Locations: Three cross-sections per titanium rod (both ends + middle), with three evenly distributed measurement points on each cross-section.
Inspection Parameters: Core measurement is Ra (arithmetic mean deviation of the profile), with Rz (maximum profile height) measured for some high-end parts.

Step 3: Dimensional Accuracy Inspection (Critical Release Indicator, Full Coverage)
The core of the inspection is "diameter, roundness, cylindricity, straightness, and length." Tools must be calibrated regularly (calibration cycle ≤ 3 months) to avoid errors.
Diameter Inspection
Inspection Tools: Outside micrometer (small diameter φ3-30mm, accuracy 0.001mm), caliper (large diameter φ30-300mm, accuracy 0.01mm)
Inspection Rules: Take 3 cross-sections per rod (100mm from both ends + middle), measure in 2 perpendicular directions at each cross-section.
Acceptance Standard: Tolerances are as per agreement; typical tolerances: normal grade ±0.02mm, precision grade ±0.005mm, no positive or negative deviation exceeding the limit.
Roundness Inspection
Inspection Tools: Roundness measuring instrument (high precision) or outside micrometer (simple inspection)
Inspection Rules: Measure 4 evenly distributed points on the same cross-section, calculate the difference between the maximum and minimum values.
Acceptance Standard: Roundness error ≤ 1/2 of the diameter tolerance, typically ≤ 0.005-0.01mm.
Cylindricity Inspection
Inspection Tools: Cylindricity measuring instrument or dial indicator + V-block
Inspection Rules: Place the titanium rod on the V-block, rotate it one full turn, and measure the entire length with the dial indicator.
Acceptance Standard: Cylindricity error ≤ 3/4 of the diameter tolerance, avoiding "one end thicker than the other."
Straightness Inspection
Inspection Tools: Straight edge + feeler gauge (short ruler ≤ 1m), string method (long ruler 1-6m), straightness measuring instrument (high precision)
Inspection Rules: Place the titanium rod flat and measure the gap at the point of maximum bending along the entire length.
Acceptance Standard: Straightness ≤ 0.1mm/m, total length ≤ 0.5mm (long ruler ≤ 6m)
Length Inspection
Inspection Tools: Steel tape measure (accuracy 1mm), vernier caliper (short ruler)
Acceptance Standard: Length tolerance ±1-5mm (as per agreement), no end skew.

Step 4: Non-destructive testing (to identify internal/surface hidden defects)
After grinding the industrial-grade titanium rods, the focus is on inspecting for grinding cracks and subcutaneous inclusions. Testing items are selected according to the grade.
Eddy current testing (ET, mandatory)

Ultrasonic testing (UT, performed as needed)

Magnetic particle testing (MT, performed as needed)

Specialized Surface Cleanliness Inspection (Medical Specific)
Detection purpose: To remove residual debris, coolant, and oil stains, preventing infection after implantation.

Step 5: Non-destructive testing (100% full inspection, higher level)

Step 6: Physicochemical and passivation film testing (medical core component)

Step 7: Sterility and biosafety testing (medical access criteria)

Step 8: Sterile packaging + traceability records (final inspection and release)

info-800-800Dia6mm Gr5Eli ASTM F136 Titanium Medical Rod manufacturers

Baoji Reliab Metal Materials Co.,Ltd

Mobile: 0086 13092900605

Sales Department 1: WhatsApp +8613092900605 (Mr.Gary)

garychen3215@hotmail.com

Sales Department 2: +8613092913521(Ms. Sophia)

boantj@163.com

Address: No.35 Baoti Rd, Weibin District, Baoji, China

 

Send Inquiry
Contact Us
    • Baoji Reliab Metal Materials Co.,Ltd
    • Mobile:+8613092900605
                     +8613092913521
    • E-mail:garychen3215@hotmail.com
                     boantj@163.com
    • Web:www.reliabmetal.com
    • Address:No.35 Middle of Baoti Road, Hi-Tech Development Zone, Baoji city, Shaanxi province China 721000